Specifying 2024 aluminum alloy (UNS A92024) provides aerospace and mechanical engineers with a premier high-strength aluminum-copper-magnesium (Al-Cu-Mg) material engineered for cyclic tension and damage tolerance. Delivering an ultimate tensile strength (UTS) of 470 MPa (68.2 ksi) and plane-strain fracture toughness (KIC) of 37 MPa·√m (33.7 ksi·√in) in the T351 temper, it resists fatigue crack propagation across flight-critical structures.
Executive Summary & Engineering Takeaways (BLUF)
- Temper & Residual Stress Control: Specify stretch-relieved 2024-T351 plate (1.5%–3.0% permanent set, yield 325 MPa / 47.1 ksi) or artificially aged 2024-T851 (yield 450 MPa / 65.3 ksi) whenever CNC pocketing removes >30% billet volume; un-stretched 2024-T3 and 2024-T4 bow up to 0.40 mm (0.016″) upon clamping release.
- Damage-Tolerant Fracture Advantage: With plane-strain fracture toughness KIC = 37 MPa·√m (33.7 ksi·√in) versus 26 MPa·√m (23.7 ksi·√in) for 7075-T651, 2024-T351 tolerates a 2.03× larger critical crack length (7.18 mm / 0.283″ vs. 3.54 mm / 0.139″) under 220 MPa (31.9 ksi) cyclic flight tension.
- Machining & Corrosion Protection Baseline: High-rake 3-flute DLC/ZrN solid carbide milling (Vc = 280–450 m/min / 920–1,475 SFM) holds general unnoted features per ISO 2768-mK and precision bored datums to ±0.010 mm (±0.0004″), paired with mandatory MIL-DTL-5541 Type II or MIL-A-8625 Type III protection.
- Ex-Factory Turnaround & Verification: Standard ex-factory production and inspection turnaround is 4 ~ 8 Business Days for bare machined parts (Ra 0.8–1.6 µm / 32–63 µin) and 7 ~ 12 Business Days for chromated or anodized parts (excluding 3 ~ 5 Days air transit), verified via Mill Test Report (MTR) traceability, ASTM E18 hardness checks, and 20 °C ± 1 °C Zeiss Coordinate Measuring Machine (CMM) inspection.
Article Engineering Navigation
- 1. Metallurgical Composition & Al₂CuMg Hardening
- 2. 2024 Tempers: T3 vs. T351 vs. T4 vs. T851
- 3. Fracture Toughness Math: 2024-T351 vs. 7075-T651
- 4. Benchmark: 2024-T351 vs. 7075-T651 vs. 6061-T651
- 5. CNC Machining Parameters & Pocket Strategies
- 6. Corrosion Mitigation: Alclad, Chem Film & Anodizing
- 7. Engineering Limitations & Metrology Protocols
- 8. Technical Engineering FAQ
1. Metallurgical Composition & Al₂CuMg Precipitation Hardening Mechanics
2024 aluminum alloy is a heat-treatable wrought aluminum-copper-magnesium alloy containing 3.8% to 4.9% copper, 1.2% to 1.8% magnesium, and 0.3% to 0.9% manganese at a density of 2.78 g/cm³ (0.100 lb/in³). This specific copper-to-magnesium stoichiometry precipitates nanoscale S’ (Al₂CuMg) and θ’ (Al₂Cu) intermetallic phases that pin dislocation slip bands under high-cycle fatigue loading.
Achieving peak mechanical integrity requires solution heat treatment at 493 °C ± 5 °C (920 °F ± 9 °F) to dissolve copper and magnesium into a supersaturated α-aluminum solid solution, followed by cold-water quenching within 15 seconds. Subsequent room-temperature natural aging or elevated-temperature artificial aging nucleates Guinier-Preston-Bagaryatsky (GPB) zones that govern yield strength and machining chip segmentation.
- Copper (3.8%–4.9% wt): Primary strengthening solute that forms coherent Cu-Mg co-clusters and semi-coherent S’ (Al₂CuMg) laths, elevating ultimate tensile strength to 470–485 MPa (68.2–70.3 ksi) while lowering baseline electrode potential and weldability.
- Magnesium (1.2%–1.8% wt): Accelerates natural aging kinetics at 20–25 °C (68–77 °F) by shifting the precipitation sequence from binary θ’ (Al₂Cu) plates toward finer, fatigue-resistant S’ (Al₂CuMg) needles within 96 hours of quenching.
- Manganese (0.3%–0.9% wt): Forms sub-micron Al₂₀Cu₂Mn₃ dispersoids that inhibit grain boundary recrystallization during hot rolling, preserving elongated fibrous grains along the longitudinal (L) rolling direction to boost fracture toughness.
- Iron & Silicon Impurity Caps (≤ 0.50% Fe, ≤ 0.50% Si): Strictly bounded under AMS-QQ-A-250/4 and ASTM B209 because insoluble coarse Al₇Cu₂Fe and Mg₂Si constituent particles act as micro-void nucleation sites under cyclic tensile stress.
2. What Is the Difference Between 2024-T3, 2024-T351, 2024-T4, and 2024-T851 Tempers?
The primary difference between 2024-T3, 2024-T351, 2024-T4, and 2024-T851 tempers lies in post-quench mechanical stress relief and aging thermal kinetics. While T3 and T4 rely on natural aging at 20 °C (68 °F) without bulk stress relief, T351 and T851 plates undergo a 1.5% to 3.0% permanent tensile stretch that eliminates asymmetric computer numerical control (CNC) machining warpage.
When machining monolithic aerospace bulkheads or multi-pocket housings removing over 40% billet volume, un-stretched 2024-T3 sheet or 2024-T4 extruded bar springs inward or bows by 0.15 to 0.40 mm (0.006″ to 0.016″). As shown in the pocketed bulkhead setup below, stretched 2024-T351 plate holds datum flatness within ⏥ 0.020 mm (0.0008″), whereas aged 2024-T851 boosts yield to 450 MPa.

For thermal stress-relief annealing limits (150–165 °C for 6061-T6 vs. ≤ 100–110 °C for 2024-T351/7075-T651) and thermal drift math (ΔL = α · L · ΔT), consult our guide on preventing deformation and residual stress in CNC milling aluminum.
| Temper & AMS / ASTM Spec | Thermomechanical Processing Route | UTS / 0.2% Yield Strength | Elongation & Hardness | ST-Axis SCC Threshold | Recommended Application / When to Choose |
|---|---|---|---|---|---|
| 2024-O (AMS 4035 / ASTM B209) | Full furnace anneal at 413 °C (775 °F) with controlled slow cooling (≤ 28 °C/hr to 260 °C) | ≤ 220 MPa (32.0 ksi) / ≤ 95 MPa (14.0 ksi) | 18%–22% / 47 HB | Not applicable (low strength) | Severe cold sheet stamping or tight-radius bending (R = 1.0t–1.5t) prior to solution heat treatment; avoid for direct finish CNC machining due to gummy built-up edge. |
| 2024-T3 (AMS 4037 Sheet) | Solution heat-treated (493 °C), cold-worked (~1% flattening), and naturally aged at 20 °C | 483 MPa (70.0 ksi) / 345 MPa (50.0 ksi) | 16%–18% / 120 HB | ~55 MPa (8.0 ksi) | Thin aerospace fuselage skins, shear webs, and laser/waterjet-profiled sheet brackets (≤ 6.35 mm / 0.250″); high warping risk if deeply pocket-milled. |
| 2024-T351 (AMS-QQ-A-250/4 Plate) | Solution heat-treated, stress-relieved by 1.5%–3.0% permanent tensile stretch, naturally aged | 470 MPa (68.2 ksi) / 325 MPa (47.1 ksi) | 18%–20% / 120 HB | ~55 MPa (8.0 ksi) | Primary shop-floor standard for CNC-milled wing ribs, tension clevis lugs, and monolithic structural bulkheads requiring ⏥ 0.020 mm flatness stability. |
| 2024-T4 / T3511 (AMS 4120 Bar / Extrusion) | Solution heat-treated and naturally aged without cold work (T4) or stretch-straightened (T3511) | 470 MPa (68.2 ksi) / 325 MPa (47.1 ksi) | 19%–20% / 120 HB | ~55 MPa (8.0 ksi) | Axisymmetric CNC-turned shafts, hydraulic couplings, and threaded aerospace fasteners from round bar; specify T3511 over un-stretched T4 for eccentric mill-turn parts. |
| 2024-T851 (AMS-QQ-A-250/4 / AMS 4268 Plate) | Solution heat-treated, 1.5%–3.0% stretched, and artificially aged at 190 °C (375 °F) for 12 hrs | 485 MPa (70.3 ksi) / 450 MPa (65.3 ksi) | 6%–8% / 128 HB | ≥ 210 MPa (30.5 ksi) | High-yield structural fittings, elevated-temperature aerodynamic skins (up to 150 °C / 302 °F), and thick-plate parts requiring superior short-transverse SCC immunity and crisp chip breaking. |
3. Why Specify 2024-T351 Over 7075-T651 for Tension Spars? Fracture Toughness Derivation
Aerospace engineers specify 2024-T351 (UTS 470 MPa / 68.2 ksi) over higher-strength 7075-T651 (UTS 572 MPa / 83.0 ksi) for lower-wing tension spars and clevis lugs because 2024-T351 delivers 42% higher plane-strain fracture toughness (KIC = 37 vs. 26 MPa·√m). Under cyclic flight tension, critical flaw length scales with KIC squared, doubling structural damage tolerance.
1. Physical Meaning & Boundary Conditions: In linear-elastic fracture mechanics (LEFM), catastrophic fast fracture occurs when the mode-I stress intensity factor KI = Y · σmax · √(π · a) reaches plane-strain fracture toughness KIC. Consider a 20 mm (0.787″) thick clevis tension lug with a reamed Ø16 mm (0.630″) pin bore machined in the longitudinal-transverse (L-T) grain orientation:
- 2. Variable Definitions & Units: ac = critical radial edge-crack length before unstable fast fracture (m / mm / in); KIC = L-T plane-strain fracture toughness (37.0 MPa·√m [33.7 ksi·√in] for 2024-T351 vs. 26.0 MPa·√m [23.7 ksi·√in] for 7075-T651); Y = 1.12 = free-edge through-crack geometry correction factor; σmax = 220 MPa (31.9 ksi) = peak cyclic tensile net-section stress.
- 3. Worked Shop-Floor Numerical Comparison:
• 2024-T351 Critical Crack Size: KIC / (Y × σmax) = 37.0 / (1.12 × 220) = 37.0 / 246.4 = 0.150162 √m → squaring gives 0.022549 m → dividing by π (3.14159) yields ac(2024) = 0.007178 m = 7.18 mm (0.283″).
• 7075-T651 Critical Crack Size: KIC / (Y × σmax) = 26.0 / (1.12 × 220) = 26.0 / 246.4 = 0.105519 √m → squaring gives 0.011134 m → dividing by π (3.14159) yields ac(7075) = 0.003544 m = 3.54 mm (0.139″).
• Damage-Tolerance Ratio: ac(2024) / ac(7075) = (37.0 / 26.0)² = 7.18 mm / 3.54 mm = 2.03× larger tolerable crack length.
4. Engineering Decision Conclusion: Specifying 2024-T351 expands the critical flaw size from 3.54 mm (0.139″) to 7.18 mm (0.283″) and slows Paris-law fatigue crack growth (da/dN) by ~3× at ΔK = 12 MPa·√m, guaranteeing that fatigue micro-cracks remain detectable during airframe field maintenance intervals long before structural failure.
Realizing this 2.03× critical crack-length advantage requires strict billet grain orientation alignment during CAM nesting, as shown in the L-direction fracture schematic below. Because rolled 2024-T351 plate has a short-transverse (ST) stress-corrosion cracking (SCC) threshold of 55 MPa (8.0 ksi) versus 240 MPa (34.8 ksi) longitudinally (L), primary tension loads must never act across the ST axis.

4. Aerospace Aluminum Benchmark: 2024-T351 vs. 7075-T651 vs. 6061-T651
Comparing 2024-T351, 7075-T651, and 6061-T651 establishes the structural triad across aluminum alloys in CNC machining. While 6061-T651 (yield 276 MPa / 40.0 ksi) provides the most economical, weldable, and corrosion-resistant baseline, 2024-T351 (yield 325 MPa / 47.1 ksi) governs cyclic tension fatigue, and 7075-T651 (yield 503 MPa / 73.0 ksi) dominates static compression.
Engineers evaluating 6061 vs 7075 aluminum or stress-relieved aluminum 6061-T6 vs 6061-T651 plates must weigh billet economics against fatigue life. Mill-traceable 2024-T351 plate carries a 1.35× to 1.55× raw material cost multiplier over 6061-T651 and increases carbide flank wear by 20%, yet its 140 MPa (20.3 ksi) endurance limit at 5×10⁸ cycles prevents vibration cracking.
| Engineering Parameter | 2024-T351 (Al-Cu-Mg) | 7075-T651 (Al-Zn-Mg-Cu) | 6061-T651 (Al-Mg-Si) | Recommended Application / When to Choose |
|---|---|---|---|---|
| Primary Strengthening Phase | Cu (3.8%–4.9%) + Mg (1.2%–1.8%) → S’ (Al₂CuMg) | Zn (5.1%–6.1%) + Mg (2.1%–2.9%) → η’ (MgZn₂) | Mg (0.8%–1.2%) + Si (0.4%–0.8%) → β” (Mg₂Si) | Choose 2024-T351 when dislocation slip reversal and crack-tip plasticity under cyclic tension govern component survival. |
| Ultimate Tensile Strength (UTS) | 470 MPa (68.2 ksi) | 572 MPa (83.0 ksi) | 310 MPa (45.0 ksi) | Choose 7075-T651 when static peak load and thin-wall elastic buckling resistance take priority over crack arrest. |
| 0.2% Offset Yield Strength | 325 MPa (47.1 ksi) (450 MPa in T851) | 503 MPa (73.0 ksi) | 276 MPa (40.0 ksi) | Upgrade from 2024-T351 to 2024-T851 when design stress exceeds 300 MPa (43.5 ksi) and ST-axis SCC immunity is required. |
| Fracture Toughness KIC (L-T) | 37 MPa·√m (33.7 ksi·√in) | 26 MPa·√m (23.7 ksi·√in) | 29 MPa·√m (26.4 ksi·√in) | Mandatory 2024-T351 selection for lower-wing tension spars, fuselage frames, and pinned clevis lugs under flight vibration. |
| Fatigue Strength (5×10⁸ Cycles, R = -1) | 140 MPa (20.3 ksi) | 159 MPa (23.0 ksi) (notch-sensitive) | 97 MPa (14.0 ksi) | In notched or bolted structures (Kt ≥ 2.5), 2024-T351 outlasts 7075-T651 due to 3× slower Paris-law crack growth. |
| Density & Elastic Modulus | 2.78 g/cm³ (0.100 lb/in³) / 73.1 GPa (10,600 ksi) | 2.81 g/cm³ (0.102 lb/in³) / 71.7 GPa (10,400 ksi) | 2.70 g/cm³ (0.0975 lb/in³) / 68.9 GPa (10,000 ksi) | 2024-T351 offers 6.1% higher elastic stiffness (73.1 GPa) than 6061-T651, reducing beam deflection in cantilevered arms. |
| Thermal Conductivity & CTE (20–100 °C) | 121 W/(m·K) / 23.2 µm/(m·K) | 130 W/(m·K) / 23.4 µm/(m·K) | 167 W/(m·K) / 23.1 µm/(m·K) | Choose 6061-T651 for high-heat-flux cold plates and electronics chassis requiring 167 W/(m·K) thermal dissipation. |
| Weldability & Uncoated Corrosion | Non-weldable (TIG/MIG) / Poor (requires Chem Film/Anodize) | Non-weldable (TIG/MIG) / Poor–Moderate (T7351 for SCC) | Excellent (ER4043/5356) / Excellent atmospheric/marine | Choose 6061-T651 whenever structural sub-assemblies require TIG/MIG welding or cosmetically uniform dyed Type II anodizing. |
5. CNC Machining Parameters, Chip Control & Thin-Wall Pocket Strategies
CNC machining 2024 aluminum alloy (rated at 70% to 80% machinability relative to C360 brass) requires high-shear positive rake geometry (15° to 20°) and polished 3-flute valleys to evacuate continuous chips. Because its copper-rich matrix contains abrasive Al₂CuMg intermetallics, high-speed steel (HSS) wears rapidly compared to diamond-like carbon (DLC) or zirconium nitride (ZrN) carbide tools.
In our in-house CNC machining facility practice on Brother Speedio and Fanuc RoboDrill 3-axis and 4-axis vertical machining centers, milling 85%-pocketed 2024-T351 wing-rib truss brackets (shown below) requires two-stage staging. We rough leaving 0.50 mm (0.020″) stock, rest 4 hours at 20 °C (68 °F), and maintain R ≥ 1/8×depth radii to curb L³/D⁴ deflection in sharp corners.

| Machining Operation | Tooling Substrate & Geometry | Cutting Speed (Vc) | Feed per Tooth / Rev (fz / fn) | Axial (ap) & Radial (ae) Cut | Recommended Application / When to Choose |
|---|---|---|---|---|---|
| Dynamic Trochoidal Roughing | 3-Flute Solid Carbide, 45° variable helix, ZrN or DLC coated, chipbreaker flutes | 280–400 m/min (920–1,310 SFM) | 0.08–0.16 mm/tooth (0.0031–0.0063 IPT) | ap = 1.5–2.0 × D / ae = 0.10–0.15 × D | High-MRR pocketing of 2024-T351 structural plates; maintains low radial cutting force to prevent thin-wall web deflection. |
| High-Speed Wall & Floor Finishing | 3-Flute Ultra-Polished Carbide or PCD End Mill, 18° positive rake, wiper flat | 350–480 m/min (1,150–1,575 SFM) | 0.04–0.08 mm/tooth (0.0016–0.0031 IPT) | ap = 1.0–1.5 × D / ae = 0.20–0.30 mm (0.008″–0.012″) | Achieving Ra 0.4–0.8 µm (16–32 µin) on fatigue-critical spar webs and mating datum pads without abrasive hand polishing. |
| Precision CNC Turning (OD / ID) | Sub-micron K10/K20 Polished Carbide or PCD Insert (CCGT/DCGT), 20° rake | 300–450 m/min (985–1,475 SFM) | 0.08–0.22 mm/rev (0.0031–0.0087 IPR) | ap (rough) = 1.5–3.0 mm / ap (finish) = 0.20–0.40 mm | Turning 2024-T4 / T3511 aerospace bushings, hydraulic pistons, and threaded couplings on Star Swiss and Takisawa lathes. |
| Peck Drilling & H7 Bore Reaming | 135° Split-Point Internal-Coolant Carbide Drill + 6-Flute Straight Carbide Reamer | Drill: 120–180 m/min (395–590 SFM) Ream: 30–50 m/min (100–165 SFM) | Drill: 0.12–0.25 mm/rev Ream: 0.15–0.30 mm/rev | Peck depth = 1.0 × D / Ream stock = 0.15 mm (0.006″) radial | Precision coaxial clevis pin bores (+0/+0.018 mm on Ø16 mm H7) requiring 40–70 bar (580–1,015 psi) through-spindle coolant. |
- Built-Up Edge (BUE) & Surface Smearing (Ra > 1.6 µm / 63 µin): Caused by low feed per tooth (fz < 0.025 mm / 0.001″) rubbing the ductile copper-aluminum matrix; correct by switching to DLC-coated (μ < 0.10) 3-flute carbide, raising fz to 0.06–0.12 mm/tooth (0.0024–0.0047 IPT), and maintaining 8%–10% Brix emulsion flood coolant.
- Continuous Chip Bird-Nesting in Deep Bore Drilling: Caused by 2024-T351’s 18%–20% elongation producing unbroken helical ribbons; correct by programming G83/G73 chip-breaking pecks every 1.0 × D depth with 40–70 bar (580–1,015 psi) through-spindle coolant, or specifying 2024-T851 where 6%–8% elongation segments chips naturally.
- Asymmetric Thin-Wall Bowing (> 0.05 mm / 0.002″ per 100 mm): Caused by machining deep pockets completely from one side; correct by executing balanced “flip-flop” roughing across Datum A and Datum B, leaving 0.40 mm (0.016″) semi-finish stock prior to unclamping and skim-finishing with contoured soft jaws.
6. Corrosion Mitigation: Alclad Cladding, MIL-DTL-5541 Chem Film & Anodizing
Uncoated 2024 aluminum alloy exhibits poor atmospheric and marine corrosion resistance because copper-rich Al₂CuMg precipitates create galvanic micro-cells (-0.68 V vs. -0.84 V matrix potential) that drive intergranular pitting and exfoliation. Protecting CNC-machined 2024 components requires sacrificial Alclad pure-aluminum skins on unmilled sheet faces, MIL-DTL-5541 chromate conversion coating, or MIL-A-8625 sulfuric/chromic acid anodizing.
A frequent DFM error occurs when engineers pocket-mill Alclad 2024-T3 plate (clad with 2.5%–5.0% pure 1230 aluminum, ~0.10 mm / 0.004″ per side) and assume corrosion protection persists. Milling strips that skin and exposes the copper core (see cross-section diagram below), mandating MIL-DTL-5541 chromate conversion or masked Type III hardcoat anodizing (shown on the H-beam link below).

Because copper reduces 2024 Type III hardcoat microhardness (380–440 HV0.05 vs. 450–550 HV0.05) while 50/50 oxide growth (25 µm inward/outward) shrinks bores by 0.05 mm, see our aluminum anodizing cost and specification guide.

7. Engineering Limitations (When NOT to Specify 2024) & Metrology Protocols
Despite its superior damage tolerance, 2024 aluminum alloy must be disqualified during design for manufacturability (DFM) reviews whenever an assembly requires TIG or MIG fusion welding, tight-radius cold sheet bending, or continuous service above 120 °C (248 °F). Identifying these metallurgical boundaries early prevents weld-zone hot cracking, outer-bend fracture, and thermal over-aging in field service.
- Prohibited for TIG / MIG Fusion Welding: The wide solidification range (502 °C–638 °C / 935 °F–1,180 °F) of the copper-rich eutectic induces severe intergranular liquation cracking along the heat-affected zone (HAZ); design 2024 joints for mechanical fasteners/rivets or substitute weldable 6061-T6 or 5083-H116.
- Unsuitable for Tight Cold Sheet Bending (Rmin < 3.0t–6.0t): Cold-forming 2024-T3 or T351 sheet (120 HB) over bend radii tighter than 3.0× to 6.0× material thickness fractures the outer tensile fibers; form in annealed 2024-O (Rmin = 1.0t–1.5t) followed by heat treatment, or specify 5052-H32.
- Unsuitable for Uncoated Marine Immersion or >120 °C Service (T351): Unprotected 2024 suffers rapid intergranular pitting in salt spray (ASTM B117), while sustained exposure above 120 °C (248 °F) coarsens S’ precipitates in T3/T351; select 2024-T851 (stable to 150 °C / 302 °F) or 6061-T651 for marine hardware.
Every production lot across our aerospace precision manufacturing, multi-axis CNC milling, and protective surface finishing lines is verified against certified Mill Test Reports (MTRs) for chemical composition and ASTM E18 hardness before machining. Following a 20 °C ± 1 °C thermal soak per our CMM metrology verification guide, ex-factory turnaround is 4 ~ 8 Business Days bare and 7 ~ 12 Business Days finished.
8. Technical Engineering FAQ
Can 2024 aluminum alloy be TIG or MIG welded for structural assemblies?
No, 2024 aluminum alloy is non-weldable by conventional TIG or MIG fusion processes because its 3.8% to 4.9% copper content causes severe hot cracking during solidification. Engineers must join 2024 components using mechanical fasteners, aerospace rivets, or switch to weldable 6061-T6 aluminum.
Why should you specify 2024-T351 instead of 2024-T3 for CNC pocket milling?
Standard 2024-T3 retains high internal quenching stresses that release unevenly during heavy CNC pocket milling, causing thin walls and flanges to bow out of flatness. Specifying 2024-T351 provides plate stretched 1.5% to 3.0% to neutralize bulk residual stress and maintain ⏥ 0.020 mm (0.0008″) datum flatness.
Does anodizing reduce the fatigue strength of 2024 aluminum aerospace parts?
Thick Type III hardcoat anodizing (25 to 50 µm) forms a brittle ceramic oxide layer whose natural micro-cracks act as stress concentrators, reducing high-cycle fatigue life by 10% to 20%. For fatigue-critical 2024 tension fittings, specify MIL-DTL-5541 chromate conversion or thin chromic/sulfuric anodizing under 10 µm.
What CNC machining tolerances and lead times are achievable for 2024 aluminum?
Our in-house CNC machining facility holds general unnoted features per ISO 2768-mK and precision bored datums to ±0.010 mm (±0.0004″) on 2024-T351 parts. Standard ex-factory production and CMM inspection turnaround is 4 to 8 business days for bare prototypes and 7 to 12 business days finished.
Ready to Machine Your Custom 2024-T351 & 2024-T851 Aluminum Components?
Whether you are validating a single 2024-T351 aerospace tension clevis from solid stretched billet or scaling to low-volume 4-axis production with custom soft-jaw fixturing, MIL-DTL-5541 conversion coating, and Zeiss CMM inspection, our in-house engineering team delivers full DFM feedback and material traceability.
Upload Your 3D CAD for DFM & Quote →